Ingeniería Civil y Mecánica
URI permanente para esta comunidadhttp://repositorio.uta.edu.ec/handle/123456789/898
Examinar
3 resultados
Resultados de la búsqueda
Item type:Ítem, Influencia del polvo de lijado y viruta de cuero en las propiedades mecánicas y de retracción por fraguado en morteros de cemento hidráulico(Universidad Técnica de Ambato-Facultad de Ingeniería Civil y Mecánica-Carrera de Ingeniería Civil, 2026-01-28) ;Analuisa Lalaleo Richard David ;Ramírez Cabrera Wladimir JoséUniversidad Técnica de Ambato-Facultad de Ingeniería Civil y Mecánica-Carrera de Ingeniería CivilThis research evaluates the influence of leather buffing dust (BD) and chrome shaving waste (CS), residues generated by the leather tanning industry, on the mechanical properties and earlyage shrinkage behavior of hydraulic cement mortars. The study emerges as a technical and environmental alternative to the high generation of solid waste from the leather industry and the growing need for more sustainable construction materials. The methodology was structured into three main phases: (i) physicochemical characterization of both residues, which revealed high contents of organic matter, nitrogen, and total chromium; (ii) particle size analysis, water absorption assessment, and mortar mix design; and (iii) mechanical performance analysis through compressive, flexural, and indirect tensile strength tests, as well as the evaluation of plastic shrinkage cracking behavior. The results showed opposing behaviors between the two residues. The incorporation of CS as an additive improved mechanical performance at low dosages. At 1 kg/m³, compressive strength increased by 23%, flexural strength by 39.5%, and tensile strength by 24% compared with the control mortar. Likewise, CS significantly reduced plastic cracking, decreasing crack length between 33% and 80%, depending on the dosage, with 10 kg/m³ identified as the most effective formulation for crack mitigation. The dominant mechanism was crack-bridging and fibrous reinforcement in both the plastic and hardened states. In contrast, the partial replacement of sand with BD resulted in severe reductions in all mechanical properties: losses ranged from 75% to 97% in compressive strength, 81% to 98.5% in flexural strength, and 63% to 96% in tensile strength. It’s very low bulk density, high water absorption, and morphology produced porous matrices, loss of granular skeleton, and poor paste–particle adhesion. Additionally, BD increased the organic load of the mortar and contributed the highest chromium content; even after cementitious immobilization, several mixes exceeded the TCLP limit, identifying BD as an unfeasible material for use in plastering mortars in its raw state. The findings indicate that the research hypothesis is validated for CS but rejected for BD. CS, used at low dosages, enhances mechanical performance and controls early-age cracking without compromising chemical stability. Conversely, BD is not suitable as a fine aggregate replacement, as it negatively affects strength, microstructure, and environmental safety of the mortar.Item type:Ítem, Correlación entre las propiedades físico-mecánicas del mortero de cemento Portland y el mortero de cal estabilizado con almidón de arroz(2020) ;Pico Sánchez, Víctor AlejandroPortilla Yandún, Favio PaúlThis paper investigates the incidence of rice starch applied to a lime mortar, in addition to replicating the process used in the construction of the Chinese wall, dosing a mortar that accomplish the specifications of “O” type glue mortar of 24 Kilograms per square centimeter at 28 days. For that reason the dosage of three types of mortars was carried out: normal lime mortar (1:2 dosage) MNC 1:2, lime mortar stabilized with sticky rice (1:2 dosage) MCEA 1:2 and cement mortar (dosage 1:5) MCP 1:5. The partial replacement of rice starch in the volume of water of the mash is crucial to determine the optimum percentage of rice starch to be used. A range of 0,5 percent to 4,0 percent of additive was used, with variation of 0,5 percent being subjected to compression tests each lime mortar with that variation of additive to identify the optimal percentage. The inclusion of rice starch in the lime mortar increases the compressive strength by the chemical reaction that occurs between calcium carbonate (hydraulic lime) and amylopectin being an abundant component in rice. The lime mortar stabilized with rice starch MCEA 1:2 has a resistance of 25,52 Kilograms per square centimeter so that accomplish the characteristics of a mortar of glue “O” type that have 24 Kilograms per square centimeter at 28 days.Item type:Ítem, Diseño y construcción de una secadora de arenas para la producción de morteros en la hormigonera Hormicen(Universidad Técnica de Ambato. Facultad de Ingeniería Civil y Mecánica. Carrera de Ingeniería Mecánica, 2018) ;Ortega Castro, Andrés SebastiánGuamanquispe Toasa, Jorge PatricioThe technical Project is based on the design and construction of a dryer of sands for the production of mortars in the cement mixer HORMICEN, to ensure the design of the dryer was carried out research on the different elements of machine, such as: burners, types of industrial dryers, as well as fuel types, composition of sand, aggregates and mortars, types of mortars, among other fundamental aspects for the implementation of the project. Next is to take all the specifications given by the concrete mixer including the sizing, the load capacity, production volumen, operating time, ease of handling, maintenance, among others. This was a grain size analysis of sand through technical specifications [10] and compared to standards suitable for this purpose (ASTM C33), the importance of the rudimentary process automation to increase the volume of production [1]. The importance of the creation of an industrial dryer is already used in different materials for sand as in our case, the most important is the removal of moisture from the material in partially low percentages. The drying of the sand for the production of dry mortar lies in that sand is exposed to environmental conditions in which moisture is directly involved with the material, the moisture makes the final result by previous processes result whit a setting of a prematurely, causing so the product does not serve for the construction. Once all the aspects of design and analysis was carried out the construction of all the constituent elements of the dryer. Whit the tests to check the operation of the machine was obtained the expected results and the satisfaction of the company.